Why is my epoxy still sticky?

Epoxy cures by a chemical reaction between resin and hardener, not by drying. If it's still tacky long after the data sheet says it should be hard, something stopped that reaction. Where the tack is tells you what.

First, check the clock

Many casting and deep-pour epoxies are slow on purpose. Compare against your product's data sheet before you assume something is wrong:

ProductPublished time
TotalBoat TableTopTack-free 6 h, sandable 24 h (1/4 in at 70 °F)
EcoPoxy UVPoxyTacky in 4–10 h, cure 48 h
MAS Deep Pour XTack-free about 12 h, sandable 24 h (2–3 in at 77 °F)
Entropy CCR + CCS SlowTack-free in 72 h at 95 °F
EcoPoxy FlowCastDemold in 3 days, cure 7–14 days

Small or thin pours of deep-pour epoxy cure more slowly than the data sheet's test casting, because they don't build up as much heat. EcoPoxy says this about FlowCast, and Let's Resin says pours under 12 fl oz of its Deep Pour cure more slowly.

Sticky spots or streaks: mixing

Soft patches, gummy streaks or a sticky ring where the cup was scraped out mean some resin or hardener never got mixed in. Unmixed material clings to the sides and bottom of the cup and to the stir stick. When you scrape the cup onto the piece, it goes on unreacted and stays soft for good.

  • Mix for the full time the data sheet gives, scraping the sides and bottom.
  • For larger batches, pour into a second clean container and mix again.
  • Don't scrape the last of the cup onto the work.

Sticky all over: ratio or temperature

Wrong ratio. Resin and hardener react in a fixed proportion. Extra of either part has nothing to react with and stays in the piece as a soft, tacky film. More hardener doesn't make it cure faster. 2:1 by volume is not 2:1 by weight; measure by the basis the data sheet gives. The mix ratio calculator splits a batch into Part A and Part B by volume and weight.

Too cold. The reaction slows as temperature drops and can stall below the product's range. WEST SYSTEM gives a 60 °F minimum cure temperature for 105/207; TotalBoat TableTop lists 65–80 °F; System Three MirrorCast 70–85 °F. A cold slab or a cold concrete floor pulls heat out of a thin coat even if the air is warm.

Waxy or greasy film: amine blush

A waxy, greasy or cloudy film on a surface that's otherwise hard is amine blush, not uncured epoxy. It forms in cool, damp conditions and can stop the next coat from bonding. Wash it off with clean water and an abrasive pad (WEST SYSTEM), dry it, then sand. Stay at least 5 °F above the dew point and skip fuel-burning heaters, which add moisture (Sherwin-Williams).

How to fix it

  • Slow but even cure: warm the room into the product's range and give it time.
  • Soft spots or tacky all over after the full cure time: it won't cure later. Scrape off the soft material, wipe the residue off with a solvent the data sheet allows, sand to a firm surface and recoat with a correctly measured, well-mixed batch.
  • Blush: wash, dry, sand, recoat.

Split 1 qt of TableTop into A and B

Sticky epoxy questions

Will sticky epoxy eventually harden?

If it's curing evenly but slowly because the room is cold, yes, once it's warm enough. If it's still tacky after the data sheet's full cure time, or only in spots, the mix was off and it won't harden. Scrape it off and recoat.

Can I pour fresh epoxy over a sticky layer?

Not over uncured material. The new coat can cure on top while the soft layer stays soft underneath. Remove the soft epoxy down to a firm surface, then sand and recoat.

Can I add more hardener to make epoxy cure faster?

No. Extra hardener has no resin to react with and leaves the piece soft and tacky. Use the product's published ratio. For a faster cure, warm the room within the data sheet's range or use a faster product.

Why is my epoxy sticky only on the surface?

A greasy or waxy film on a hard coat is usually amine blush from cool, humid air. Wash it off with water and an abrasive pad before sanding or recoating.